Skip to main content

Table 2 Mean microtensile bond strength results in MPa and (standard deviation), percentage % of pre-test failures, and number of specimens tested of the different adhesives

From: L-arginine-containing mesoporous silica nanoparticles embedded in dental adhesive (Arg@MSN@DAdh) for targeting cariogenic bacteria

Adhesives

µtbs (MPa)*

Pre-test failures (%)

Number of specimens

SB1XT

35.9 (13.9) a

23

67

SBUP

36.4 (18.7) a

31

60

Unfilled

20.0 (9.3) bc

37

61

0.5%Arg@MSNs

22.6 (9.6) b

32

64

1%Arg@MSNs

20.9 (10.3) bc

59

39

2%Arg@MSNs

15.3 (7.5) c

52

43

  1. * Different letters in the same column indicate statistically significant differences between the adhesives tested (p < 0.05)